A lot of stainless steel mig welding tests are set up using Tri mix shielding gas (90 helium - 7.5 argon-2.5 co2) and .035" 308 stainless steel mig wire.try these settings for a start and adjust from there....20 volts 300 inches per minute ( if the machine does not read in ipm, just pull the trigger and count to 6 seconds. then measure the wire that came out and multiply by 10..in this case , 30 inches of wire in 6 seconds)One suggestion if you use tri mix gas....., Old timers believe you should roll the bottle on the floor to mix it up, at the very least you should probably remove the gauge and crack the valve to blow some gas out let it churn a bit inside the tank.